KARAKTERISTIKAT TEKNIKE | METODA E TESTIMIT | STANDARD | NEX-GEN |
MATJA DHE PARAQITJA E SIPËRFAQËSISË | |||
GJATESIA DHE GJERESIA | EN ISO 10545-2 | ±0,6% | -0,01% ~+0,01% |
±2 mm | -0,05mm ~+0,04mm | ||
TRASHËSIA | EN ISO 10545-2 | ±5% | -0,11% ~+1,26% |
±0,5 mm | -0,01mm ~+0,12mm | ||
DREJTËSIA E ANËVE | EN ISO 10545-2 | ±0,5% | -0,02% ~+0,01% |
±1,5 mm | -0.1mm ~+0.08mm | ||
VETITË FIZIKE | |||
THYRTIMI I UJIT | EN ISO 10545-3 | ≤0,5% | ≤0,1% |
THYERJA E FORCËS | EN ISO 10545-4 | ≥1300N | 2204 |
MODULI I RUPTURËS | EN ISO 10545-4 | ≥35N/mm² | 49 |
REZISTENCA NDAJ gërryerjes | EN lSO 10545-7 | RAPORTI NË KLASËN E ABRAZIONIT | Klasa 3 |
CIKLET E RAPORTIT TË KALUARA | 1500 r | ||
REZISTENCA TERMIKE SHOKU | EN ISO 10545-9 | NUK DUHET TË DUHET ASNJË defekt | KALOJE |
REZISTENCA NGA NGRITJA | EN ISO 10545-12 | JO DEFEKTE SIPËRFAQËSORE OSE DUHET TË DUHEN TË PARAQITUR | KALOJE |
Rrëshqitësi 96 REZISTENCA NË RRËSHQITJE,TESTI I lavjerrësit të lagësht | SIPAS AS 4586:2013 | - | |
MATT | P3 | ||
E JASHTME | P4 | ||
VETITË KIMIKE | |||
REZISTENCA KIMIKE TE KIMIKAT E FAMILJEVE & KRIPËRA TË PISHINAVE | EN ISO 10545-13 | MINIMUM GB | A |
REZISTENCA NDAJ NJOLJES | EN ISO 10545-14 | KLASA MINIMUM 3 | KLASA 5 |
SERIA | PËRMASAT | PCS/CTN | M²/ CTN | M²/PLT | CTN / PLT | KG/PLT |
MERMER | 450x900mm/18"x36" | 3 | 1.215 | 68.04 | 56 | 1512 |
600x600mm/24"x24" | 4 | 1.44 | 57.6 | 40 | 1520 | |
600x1200mm/24"×48" | 2 | 1.44 | 74.88/43.2 | 56/30 | 1,768/1020 |
*Pllakat mund të ndryshojnë në madhësi, peshë, ngjyrë, model, lyerje, strukturë, qëndrueshmëri, dendësi, sipërfaqe dhe përfundim nga grupi në grup.Vlerësimet e rrëshqitjeve shërbejnë si tregues dhe mund të ndryshojnë për çdo grup pllakash.Rekomandohet që të kryhet një test i ri për çdo grup pllakash nëse kërkohet një certifikatë e vlerësimit të rrëshqitjes.Imazhet e treguara të produktit janë vetëm për qëllime ilustrimi dhe nuk janë një paraqitje e saktë e produktit.