CIRI Téknis | METODE UJI | STANDAR | NEX-GEN |
PANGUKURAN & TAMPILAN BUNGA | |||
PANJANG JEUNG LEBAR | EN ISO 10545-2 | ± 0,6% | -0,26% ~-0,14% |
± 2 mm | -0.8mm ~-0.4mm | ||
KETEPATAN | EN ISO 10545-2 | ± 5% | -0,4% ~+0,9% |
± 0,5 mm | 0 ~+0,1 mm | ||
STRAIGHTNESS SISI | EN ISO 10545-2 | ± 0,5% | +0,01% ~+0,03% |
± 1,5 mm | -0.1mm ~ + 0.2mm | ||
SIFAT FISIK | |||
nyerep cai | EN ISO 10545-3 | E> 10% | 17,60% |
NGAREGEPKEUN | EN ISO 10545-4 | ≥600N | 877 |
MODULUS RUPTURE | EN ISO 10545-4 | ≥12N/mm² | 26.4 |
Résistansi kana abrasion | EN lSO 10545-7 | LAPORAN KA KELAS ABRASION | KELAS 4 |
LAPORAN SIKLUS LULUS | 2.100r | ||
Résistansi CRAZING | EN ISO 10545-11 | Résistansi pinuh | LULUS |
Résistansi ibun | EN ISO 10545-12 | Résistansi pinuh | LULUS |
SIFAT KIMIA | |||
Résistansi KIMIA KA BAHAN KIMIA RUMAH TANGGA & Uyah kolam renang | EN ISO 10545-13 | MINIMUM GB | A |
Résistansi pikeun ngawarnaan | EN lSO 10545-14 LAMUN KANA BAHAN KIMIA | KELAS MINIMUM 3 | Kelas 5 |
SERI | UKURAN | PCS/CTN | M²/ CTN | M²/ PLT | CTN/PLT | KG/PLT |
Minimal | 65x265mm/3"x10" | 58 | 1 | 96 | 96 | 1344 |
* Ubin tiasa béda-béda dina ukuran, beurat, warna, pola, urat, tékstur, daya tahan, dénsitas, permukaan sareng bérés ti bets ka bets.Slip ratings ngawula ka salaku indikasi jeung bisa rupa-rupa pikeun tiap bets ubin.Dianjurkeun yén tés anyar dipigawé pikeun tiap bets ubin lamun sertipikat rating dieunakeun diperlukeun.Gambar produk anu dipidangkeun ngan ukur kanggo ilustrasi sareng sanés ngagambarkeun persis produk.